    The previous piece came out excellent but I didn't get a picture after it was completed. After it completely cured, used Plasticast and an 8hr burnout and it came out great.

    Here's the test using phosphate-bonded investment. Came out better, but not quite there. This is definitely a curing issue. Larger pieces are concealing uncured resin, and since the new material is more opaque than FTX Green, curing time may need to be extended. Thinking about building an external curing chamber.