Results 1 to 10 of 31
Threaded View
-
06-13-2016, 10:10 AM #7
- Join Date
- Jun 2016
- Posts
- 7
I tried some of the above suggestions and got the following results...
Settings: Nozzle temp 205, bed temp 50
Result: Filament came out and glommed up. Nothing would stick to the bed.
Settings: Nozzle temp 205, bed temp 60 w/glue stick on bed.
Result: Fliament came out glommed up. Nothing would stick to the bed
Settings: Nozzle temp 170, bed temp 0 w/glue stick on bed.
Result: Filament would not feed at all.
Settings: Nozzle temp 230, bed temp 0 w/glue stick on bed.
Results: Filament feeds well, sticks to bed completely. (At this time it's only about 20% completed with the print but far more successful than any previous attempts with PLA material)
Thanks again.