A couple observations.
1st: I wouldn't use a raft unless it is a part that requires it such as very limited contact with the bed. Also make sure the bed is clean. Acetone or alcohol to clean with.
2nd: Make sure the printer is enclosed and shielded from drafts such as air conditioning.
3rd: Let the machine pre-heat for a while with the bed to get the temp up in the chamber.
4th: You can start to drop the bed temp after the first layer probably down to 100. May take some experimentation.
5th: You will probably need something to help with adhesion such as hair spray or glue stick or ABS juice.
6th: Make sure the parts cooling fan is not on.
7th: Speed. Slow first layer then I would try around 2400mm/min to start with and use a .2 layer height.

When you had an issue with PLA you mention using the same temps - if it is what you used for ABS then WAY to high! PLA - 65 bed to start then drop after first layer and 200 to start on extruder.