Originally Posted by
clough42
I have been running MakerFarm ABS with Garnier Fructis Extreme Hold #5 on glass at 100/110C, and I haven't had any trouble. Keeping stray air off the bed is important. Also, I have been getting different results from different colors of filament. Black and White adhere well and are easy to control when printed at 250C. Orange doesn't adhere as well and oozes more. Clear ABS is just awful. It's brittle. It pops off the bed at the slightest provocation and oozes and strings badly. If I lower the temperatures, then I get delamination. It's voodoo.
I clean the glass with hot water and a sponge, dry it and then spray on enough hairspray to coat, but not run or drip. I then spray on another light coat after each print. It takes a print or two (with subsequent coats of hairspray) to get things sticking well. Eventually, the bed becomes rough with the outlines of previous prints, and I clean it off and start over. I probably do this every ten prints or so.